Gas Welding


Plate Thickness in mm Welding Technique Filler Rod Dia in mm O2 Consumption
in cu m/hr
Acetylene Consumption
in cu m/hr
Welding Time per meter in min Length of
Filler rod required/m
of welding
in meter

1 Leftward 1.00 0.04 0.02 9 to 11 1.0
2 " 2.0 0.10 0.04 10 to 12 1.5
3 " 2.5 0.12 0.07 12 to 13 1.6
4 " 3.0 0.15 0.10 13 to 15 2.6
5 " 3 or 4 0.21 0.14 15 to 17 4.0 or 1.8
5 Rightward 2.5 0.3 0.20 16 to 18 3.3
6 " 3.0 0.4 0.25 18 to 20 3.4
8 " 4.0 0.5 0.30 20 to 28 3.6
10 " 5.0 0.7 0.5 30 to 35 4.5
15 " 6.0 1.0 0.6 45 to 50 6.8
20 " 6.0 1.2 0.8 60 to 67 10.0
25 " 6.0 1.6 0.9 85 to 100 16.0





Plate
Thickness
in mm
Nozzle Diam.
in mm
O2 pressure kg/cm2 Consumption m2/hr Cutting Speed m/hr

Head Machine O2 C2H2

Head Machine Head Machine Head Machine

3 0.8 or 1 1.0-1.65 1.0-2.0 1.3-1.4 1.2-1.4 0.2-0.25 0.18-0.25 30-45 30-50
 
5 1 0.75-1.50 0.75-2.0 1.8-2.0 0.8-2.0 0.15-0.20 0.12-0.20 20-30 18-32
 
10 1 or 1.5 1.5-2.0 1.5-3.5 1.2-2.4 1.0-2.4 0.20-0.25 0.15-0.25 15-30 15-30
 
15 1.5 1.7-2.5 1.5-3.5 3.5-4.5 3.5-4.5 0.33-0.45 0.33-0.42 18-27 18-30
 
25 1.5 3.1-2.8 2.0-2.8 3.6-5.0 3.6-0.47 0.36-0.47 0.35-0.47 15-28 18-30