Stress Intensity Factor (KI) Calculator


Linear-elastic fracture mechanics for a through crack: mode-I stress intensity, comparison with the material fracture toughness, and the critical crack size at the applied stress.

a = half-length for a center crack, full depth for an edge crack. Y = 1.0 center, 1.12 edge.

Enter your values:
Results:

How it works

The crack-tip field scales with the stress intensity factor:

Kᵤ = Y × σ × √(πa)

with a the crack length (half-length for a center crack), σ the remote stress and Y the geometry factor (1.0 center crack in an infinite plate, 1.12 edge crack, 2/π = 0.637 for a penny-shaped embedded crack). Fracture follows when Kᵤ reaches Kᵤ₊.

Worked example

Edge crack a = 5 mm, σ = 250 MPa, Y = 1.12: Kᵤ = 1.12 × 250 × √(π × 0.005) = 35.1 MPa√m. Against Kᵤ₊ = 80 MPa√m the margin is 2.28, and the critical size is (80/(1.12×250))²/π = 26 mm.

Assumptions and limitations

  • Linear-elastic: valid while the plastic zone stays small versus the crack and the section.
  • Plane strain toughness Kᵤ₊ is conservative; thin sections give higher apparent toughness.
  • Y depends on crack and part geometry; handbooks (Tada, Rooke & Cartwright) give exact factors.