Fatigue Crack Growth Calculator (Paris Law)
Cycles to grow a crack from an initial to a final size under constant-amplitude loading, using the Paris-Erdogan law da/dN = C(ΔK)^m.
C in m/cycle with ΔK in MPa√m (steels ~1e-11 to 1e-12, m ~3). Sizes in mm.
How it works
In the stable-growth regime the crack advances by:
da/dN = C(ΔK)^m, with ΔK = Y Δσ √(πa)
Integrating from aᵢ to aₖ for m ≠ 2: N = [aₖ^(1−m/2) − aᵢ^(1−m/2)] / [(1−m/2) C (Y Δσ √π)^m]. For m = 2: N = ln(aₖ/aᵢ) / [C (Y Δσ √π)²].
Worked example
Steel, C = 6.9×10⁻¹² (m/cycle, MPa√m), m = 3, Y = 1.12, Δσ = 100 MPa, growing from 1 mm to 10 mm: Y Δσ √π = 1.12 × 100 × 1.7725 = 198.5, so N = [0.01^(−0.5) − 0.001^(−0.5)] / [(−0.5) × 6.9×10⁻¹² × 198.5³] = (10 − 31.62) / (−2.699×10⁻⁵) = 8.01×10⁵ cycles.
Assumptions and limitations
- Constant amplitude, no retardation after overloads; variable loading needs cycle-by-cycle integration.
- C and m come from test data and depend on material, R-ratio and environment; a 2× change in C halves or doubles life.
- Near-threshold and near-toughness regions do not follow the power law.