| Designation of Steel | Grade | Tensile strength kgf/mm2 | C % | Si % | Haedened in oil at oC | Annealed at oC | Typical Applications | |
|---|---|---|---|---|---|---|---|---|
| Hardened and Tempered | Annealed Max. | |||||||
| C 45 ... ... | 1 | 120-145 | 60 | 0.40-0.50 | 0.10-0.35 | 830-860 | 600-650 | In the form of bars and flats for volute, helical and leminated spring for automotive suspension |
| C 65 ... ... | 3 | 120-145 | 60 | 0.60-0.70 | 0.10-0.35 | 810-840 | 600-650 | |
| C 75 ... ... | 5 | 120-160 | 65 | 0.70-0.80 | 0.10-0.35 | 810-840 | 600-650 | |
| C 98... ... | 8 | 160-180 | 70 | 0.90-1.05 | 0.10-0.35 | 770-800 | 620-660 | |
| 55 Si 2 Mn 90 ... | 9 | 160-200 | 80 | 0.50-0.60 | 1.05-2.00 | 830-860 | 640-680 | |
| 50 Cr I ... ... | 10 | 170-230 | 80 | 0.45-0.55 | 0.10-0.35 | 830-860 | 640-680 | |
| 50 Cr IV 23 | 11 | 190-240 | 80 | 0.45-0.55 | 0.10-0.35 | 830-860 | 600-680 | |