| Designation of Steel | Properties in quenched & tempered condition | Surface hardness obtainable HRC | Hardening temperature | Typical Applications | |||
|---|---|---|---|---|---|---|---|
| Tensile range kgf/mm2 | 0.2% proof stress, Min kgf/mm2 | Izod impact Min kgf.m | For oil quench | For water quench | |||
| C 30 | 60-75 | 36 | 5.5 | 45-50 | 860-890 | 860-890 | These wrought unalloyed and alloyed steels for flame and induction hardening are used when high core strength and good impact properties are required. |
| C 45 | 70-85 | 44 | 3.5 | 55-61 | 830-860 | 820-850 | |
| T 70 | 70-85 | 40 | 2.8 | 60-63 | 810-840 | 780-810 | |
| 37 Mn 2 | 60-75 | 40 | 4.8 | 53-59 | 850-870 | 840-860 | |
| 40 Mn 2 Mo 45 | 70-85 | 46 | 4.8 | 53-59 | 850-870 | 840-860 | |
| 35 Mn 2 S 12 | 80-95 | 56 | 5.5 | 53-59 | 840-860 | 830-850 | |
| 54 Cr 1 | 80-95 | 48 | 2.8 | 57-62 | 850-870 | 840-860 | |
| 50 Cr 1 V 23 | 80-95 | 48 | 2.8 | 57-62 | 850-870 | 840-860 | |
| 40 Ni 3 | 80-95 | 56 | 5.5 | 54-60 | 830-860 | 840-870 | |
| 40 Ni 2 Cr 1 Mo 28 | 90-105 | 66 | 5.5 | 54-60 | 830-840 | 810-830 | |
| 31 Ni 3 Cr 65 Mo 55 | 90-105 | 66 | 5.5 | 49-54 | 850-880 | 820-840 | |