| Designation of Steel | Properties in hardened and tempered condition | Normalizing Temperature oC | Hardening Temperature oC | Quenching medium | Tempering Temperature oC | Typical Applications | |
|---|---|---|---|---|---|---|---|
| Tensile strength kgf/mm2 | Yield stress Min. kgf/mm2 | ||||||
| C 30 | 60-75 | 40 | 860-890 | 860-890 | Water or oil | 550-660 | These wrought unalloyed and alloyed steels in the form of billets and bars for general engineering purposes are used in the hardened and tempered condition. |
| C 35 Mn 75 | 60-75 | 40 | 850-880 | 840-880 | Water or oil | 530-760 | |
| C40 | 60-75 | 38 | 830-860 | 830-860 | Water or oil | 550-660 | |
| C 45 | 60-75 | 38 | 830-860 | 830-860 | Water or oil | 530-670 | |
| C 50 | 80-95 | 54 | 810-840 | 810-840 | Oil | 550-660 | |
| C 55 Mn 75 | 80-95 | 54 | 810-840 | 810-840 | Oil | 550-660 | |
| 40 S 18 | 70-85 | 48 | 830-860 | 830-860 | Oil | 550-660 | |
| 40 Mn 2 S 12 | 60-75 | 40 | 840-870 | 840-870 | Oil | 550-660 | |
| 20 Mn 2 | 60-75 | 44 | 860-900 | 860-900 | Water or oil | 550-660 | |
| 27 Mn 2 | 70-85 | 46 | 840-880 | 840-880 | Water or oil | 550-660 | |
| 35 Mn 2 Mo 45 | 100-115 | 80 | - | 840-860 | Oil | 550-660 | |
| 55 Cr 70 | 90-105 | 66 | 800-850 | 800-850 | Oil | 500-700 | |
| 40 Cr 1 | 80-95 | 60 | 850-880 | 850-880 | Oil | 550-700 | |
| 40 Cr 1 Mo 28 | 80-95 | 60 | 850-880 | 850-880 | Oil | 550-720 | |
| 40 Cr A 1 I Mo 18 | 90-105 | 70 | - | 850-890 | Oil | 550-700 | |
| 40 Ni 3 | 90-105 | 70 | 830-860 | 850-860 | Oil | 550-650 | |
| 35 Ni 1 Cr 60 | 90-105 | 70 | - | 820-850 | Water or oil | 550-660 | |
| 30 Ni 4 Cr 1 | 120-135 | 130 | - | 810-830 | Air or oil | upto 250 | |
| 40 Ni 2 Cr 1 Mo 28 | 120-135 | 130 | - | 830-850 | Oil | 550-660 | |
| 31 Ni 3 Cr 65 Mo 55 | 120-135 | 100 | - | 830-850 | Oil | upto 660 | |
| 40 Ni 3 Cr 65 Mo 55 | 120-135 | 130 | 830-850 | 830-850 | Oil | upto 660 | |